40CrV

Alloy Steel

40CrV

(GB/T 3077). Nominal values—confirm mill certificate.

Chemical Composition (%)

C0.37
SI0.17
MN0.5
CR0.8
V0.1
P0.035
S0.035

Mechanical Properties

Tensile:≥885 MPa;Yield:≥735 MPa;Elong:≥10%;RA:≥45%

Chinese Standard

T 3077 40CrV

Available Forms

Bar,Plate

Uses

Low-alloy engineering steel with enhanced hardenability and strength from alloying elements. Chromium (≈0.95%) improves hardenability, wear and corrosion resistance. Vanadium (≈0.15%) refines grain and strengthens the tempered structure. Applied to gears, shafts, bolts, connecting rods, pressure parts and heavy forgings in automotive, energy and machinery sectors.

Heat Treatment

Austenitize at 820–870 °C (oil or water quench depending on section) and temper at 400–650 °C to the required strength/toughness balance.

Precautions

Preheat and control interpass temperature when welding; post-weld heat treatment or stress relief is recommended to avoid hard-zone cracking. Use low-hydrogen electrodes. Protect from decarburization during heating (controlled atmosphere or protective coating).