45SiCrV6-2

Other

45SiCrV6-2 / 1.8151

45SiCrV6-2 grade supplied by Shanxi Youte Steel (jlhsteel.net).

Chemical Composition (%)

C0.4
SI1.3
MN0.6
P0.025
S0.025
CR0.4
V0.1

Available Forms

Bar, Plate, Tube, Forging

Uses

Spring steel with high elastic limit and fatigue strength for coils, leaf springs, clips and suspension parts. Silicon (≈1.5%) raises elastic limit and tempering resistance. Supplied as strip, wire and bar; shot-peened after forming for longer service life.

Heat Treatment

Austenitize 830–880 °C (oil quench) and temper at 400–520 °C; stress-relieve formed springs at 230–320 °C after coiling.

Precautions

Preheat and control interpass temperature when welding; post-weld heat treatment or stress relief is recommended to avoid hard-zone cracking. Use low-hydrogen electrodes. Protect from decarburization during heating (controlled atmosphere or protective coating). Shot-peen after coiling to improve fatigue life; avoid sharp bends and surface defects.